1. The numbers this group shares
| Parameter | Setting |
|---|---|
| Tunnel set temperature | 175 ℃ |
| Working window | 160–180 ℃ |
| Shrink initiation, lower limit | 150 ℃ |
| Machine-direction shrinkage | 68 % |
| Transverse-direction shrinkage | 14 % |
| Seal strength | ≥12 N/15 mm |
| Light transmission after shrinkage | ≥90 % |
| Puncture resistance | 30 % above standard beverage film |
| Line speed, seal time, cooling time, dwell | Locked to the nameplate at first-off |
| Film capability envelope | 30–300 μm, width 100–2000 mm, MD 65–80 %, TD 0–25 %, best at 160–180 ℃ |
Three are working values: 68 % MD, 14 % TD, 175 ℃ tunnel. The rest are boundaries and inspection values. Figures are the customary range for the category; the delivered batch test report governs.
2. Why these numbers cannot move
Temperature has a boundary on both sides. Below 160 ℃ the film draws unevenly around cap and base, leaving slack folds read as a packing defect; above 180 ℃ it risks bursting. The upper limit differs by machine and is found on the machine, not assumed from the nameplate.
Transverse shrinkage above 14 % is the most common single cause of cap weep: the film pulls the shoulder inward and loads the cap thread while the bottle is still warm. The pack looks tightest at the exit and weeps the next day.
MD at 68 % clamps the pack vertically: enough to pull bottles onto the base pad, not enough to tear the bottom edge when the pack is lifted by one corner. Dropping MD for line speed is what produces the slack bottom pack on day two.
3. Thickness follows the pack, not the price
| Pack | Pack geometry | Film thickness |
|---|---|---|
| Carbonated 330–500 ml, 4 / 6 / 8 bottles | Round bottle, pack width 130–200 mm | 70 μm |
| Carbonated 1.25–2 L, 2 / 4 bottles | Large round bottle, height 300–330 mm | 80 μm |
| Juice 330–500 ml, 4 / 6 bottles | Square or shaped bottle | 80 μm |
| Juice 1 L, 4 / 6 bottles | Square bottle, width 176–200 mm | 90 μm |
| Concentrate or syrup drum, 20 L | Top-over bag, folded base | 100 μm |
Order the single value, not a range. Beverage-grade film spans 50–120 μm and 200–2000 mm; a pack needing more than 120 μm has entered the industrial PE range, a different specification and window rather than the same film made thicker.
An eight-pack of 500 ml takes 70 μm although it is heavier than a six-pack, because load per bottle is unchanged. A 2 L two-pack takes 80 μm because bottle mass, not bottle count, sets the film.
4. Lay-flat width: one formula, four worked examples
Lay-flat width in millimetres equals product length plus 0.66 times bottle height, rounded up to the next 10 mm:
W = L + 0.66 H
The 0.66 factor is the two end take-ups combined, about one third of the bottle height at each end. It is not a safety margin and it is not added to a pack width. Product length is the pack length along the film direction - columns times bottle diameter.
Example 1. 500 ml carbonated, eight bottles, two rows by four; Ø65 mm, height 210 mm. L = 4 × 65 = 260 mm. W = 260 + 0.66 × 210 = 398.6 mm, rounded to 400 mm. The Ruiyue 500 ml series stocks 360 / 430 / 490 / 560 mm, so 400 mm is bought as the 430 mm roll.
Example 2. 1.25 L carbonated, four bottles, two by two; Ø88 mm, height 300 mm. L = 176 mm. W = 176 + 198 = 374 mm, rounded to 380 mm, tier 430 mm.
Example 3. 2 L carbonated, two bottles in one row; Ø110 mm, height 330 mm. L = 220 mm. W = 220 + 217.8 = 437.8 mm, rounded to 440 mm, tier 490 mm.
Cross-check. 1 L juice, six bottles, two rows by three; 88 mm square, height 300 mm. L = 264 mm. W = 264 + 198 = 462 mm, rounded to 470 mm, tier 490 mm.
Two consequences follow. The formula returns a theoretical width; the width you buy is a stock tier, and the gap is paid on every pack. Less obvious: on the large-bottle branch, a two-bottle pack and a four-bottle pack two by two share the same 220 mm length and 440 mm width - the four-pack only consumes more length. Width changes only when bottles go into a single row: 4 × 110 = 440, W = 657.8 mm, past the 560 mm top, so it becomes a custom width. Bottles along the row push you off the tier table; rows do not.
Film consumption per pack follows wrapped length, K = 2 (G + H) × 1.1, where G is pack depth across the rows and H the bottle height; 1.1 covers 10 % shrinkage plus overlap. Price an orientation change on both dimensions:
500 ml eight-pack, two rows by four: 430 × 2 (130 + 210) × 1.1 = 321,640 mm². Turned to four rows by two: width 268.6, tier 360, length 1034, giving 372,240 mm² - about 16 % more.
1.25 L four-pack: 430 × 1047 = 450,296 mm². Turned to one row of four: width 550.8, tier 560, length 853.6, giving 478,016 mm² - about 6 % more.
1 L juice six-pack: 490 × 1047 = 513,128 mm². Turned to three rows by two: width 374, tier 430, length 1240.8, giving 533,544 mm² - about 4 % more.
On theoretical width alone the turned layouts look cheaper - the juice six-pack turned saves roughly 4 % of wrapped area - but once the theoretical width is pushed up to a stock tier the saving disappears and reverses. Check the tier before changing the pallet pattern, not after.
5. What the film carries
The film provides collation, dust protection, load-bearing and overall integrity. It takes the drag loads of handling and the compressive load of stacking, which is what lets a pack travel and be delivered as one unit instead of loose bottles. Pallet structure, corner protection and strapping follow the customer stacking plan and are specified separately.
6. Three failure points worth checking first
Cap weep at the thread. Film too tight at the shoulder, or TD above 14 %, loads the closure before the pack cools. It shows between 12 and 36 hours, after the pallet has been signed off.
Bottom pack out of square. Short cooling, or pallets built before residual shrinkage finishes, lets stack weight complete the job on the bottom pack.
Fog inside the film, print walking at the fold. Short forced-air cooling traps moisture inside; film packed print-face down, or vertical artwork, puts compensated print across the fold beyond what 3.125 covers.
7. Print layout and compensation
Compensated size equals finished size divided by one minus the shrinkage in that direction: at 68 % MD the factor is 1 ÷ 0.32 = 3.125, at 14 % TD it is 1 ÷ 0.86 = 1.163. Artwork therefore runs as a horizontal band along the machine direction; vertical barcode blocks are not usable at this window. Print is limited to seven colours, and compensation is confirmed at sampling rather than cut from a drawing.
8. Sampling and the three acceptance checks
Sample on your own bottle and machine at the locked settings, and hold the packs 36 hours before judging. All three checks must pass:
36-hour re-check. Pallet built and held 36 hours: bottom layer must not go out of square, no cap may weep at the thread, no continuous fog band on the inside face.
Seal and width. Seal strength ≥12 N/15 mm on the sampled batch; lay-flat width inside the tolerance of the ordered tier.
Optical and integrity. Light transmission after shrinkage ≥90 %, no burst packs, no punctures, no open fold.
FAQ
Do 500 ml six-packs and eight-packs run the same roll? No. Two rows by three gives 195 + 138.6 = 333.6 mm, so 340 mm and the 360 mm tier; the eight-pack gives 398.6 mm and the 430 mm tier. Same thickness, different roll.
Why not lay a 2 L four-pack as one row of four? Because 440 + 217.8 = 657.8 mm, past the 560 mm top of the series: a custom width with a different lead time, for no gain in protection.
Can TD be raised to 18 % so the pack looks tighter? TD is a setting, not a preference. Above 14 % the shoulder load reaches the cap thread before the pack cools, and the tight look at the tunnel exit is the symptom.
Why must print run as a horizontal band? The machine direction stretches 3.125 times at 68 %. Anything set vertically is drawn into the fold and will not scan after shrinkage.
The workshop is cold in winter - set the tunnel higher? No. The window is 160–180 ℃ with a 150 ℃ initiation floor, locked at first-off. Raising the set point for a cold workshop is how packs arrive at 180 ℃ and burst.
About Ruiyue Plastics
Ruiyue Plastics is based in Jiading, Shanghai, and runs both PE and POF shrink film lines, with separate ranges for beverage-grade and industrial-grade film. Beverage packs are quoted on the settings above, with width taken from the stock tier rather than the theoretical figure.
CTA: Request a sample run on your bottle and machine - include bottle Ø and height, bottles per pack, row arrangement, and the pallet pattern you ship on.